联众涂料论坛

标题: 环氧富锌和无机福锌漆适合划格法试验吗?? [打印本页]

作者: HJ120    时间: 2011-4-16 23:49
标题: 环氧富锌和无机福锌漆适合划格法试验吗??
如题所示,这两种漆适合做划格法试验吗?为什么?有标准依据吗?
作者: BMA004    时间: 2011-4-19 22:06
没有说不可以吧
作者: HJ120    时间: 2011-4-20 08:55
总是感觉不好!
作者: renliu521    时间: 2011-4-20 08:56
也想了解
作者: Epoxy    时间: 2011-11-17 16:13
无机锌不适合用划格法,因为颜料太多
作者: agneshawk    时间: 2011-11-18 07:45
没说不可以,看你自己的产品了,其实连水性无机富锌底漆都可以做的(可以达到0级)。
作者: shigang2006    时间: 2011-11-25 13:38
为什么我做的醇溶性无机富锌底漆表面很粗糙呢 且附着力不好
作者: 杨红波    时间: 2011-11-25 19:48
用的哪里的树脂?基础配方怎么样?
作者: ouranyujian    时间: 2011-11-29 08:16
划格不可怕,可怕的是有个项目要水性富锌花圈法到1级,如果试板处理的不合适,很容易出现问题。但是各个厂家的不同,有的厂家是附着力好,但是柔韧性差,各有优势吧。
作者: laiyangli    时间: 2011-12-6 19:39
不适合!

1. 见ISO 2409-2007:
The method is not suitable for coatings of total thickness greater than 250 μm or for textured coatings.
NOTE 2 The method, when applied to coatings designed to give a rough patterned surface, will give results which will show too much variation (see also ISO 16276-2).
2. 见ISO 16276-2-2007
The cross-cut test is suitable for film thicknesses up to 250 μm. The X-cut test is not limited by thickness.
For hard coatings, it might not be possible to use the cross-cut test, in which case the X-cut test should be
used.
For coatings containing pigments that have a flake format, the assessment of either the cross-cut or the X-cutmight be misleading. The coating manufacturer should be consulted for recommendations.
作者: wang_7njcoating    时间: 2012-1-10 10:19
不适合!
作者: wsiczhao    时间: 2012-5-9 20:36
最好都用拉拔法,TB/T 1527-2011、JT 722-2008对涂料附着力要求都是5MPa以上,普遍采用拉拔法检测。
作者: 阳光灿烂    时间: 2012-5-14 15:04
铁路标准1527,水性无机富锌划格法2级。
不过最好还是拉开法。
作者: mengjie1019    时间: 2012-6-18 14:58
我的环氧富锌,划圈一级,至于划格,不好操作啊,劲小了漆膜毫无损伤,主要感觉还是跟膜厚有关吧。
作者: zerozsh    时间: 2012-6-26 14:08
基本不推荐哦,道理我也不是太清楚哦
作者: 阳光灿烂    时间: 2012-6-26 15:50
个人体会,拿锤子砸,漆膜不掉,说明附着力没问题/:victory
作者: chenxujie    时间: 2012-7-4 08:14
shigang2006 发表于 2011-11-25 13:38
为什么我做的醇溶性无机富锌底漆表面很粗糙呢 且附着力不好

干的太快  干喷?

作者: westy    时间: 2012-8-12 22:51
一般使用拉拔法测定附着力,水性富锌漆一般用画格法测定附着力。
作者: renguangyi001    时间: 2012-9-12 15:12
不可以 。看10楼的详解
不适合!

1. 见ISO 2409-2007:
The method is not suitable for coatings of total thickness greater than 250 μm or for textured coatings.
NOTE 2 The method, when applied to coatings designed to give a rough patterned surface, will give results which will show too much variation (see also ISO 16276-2).
2. 见ISO 16276-2-2007
The cross-cut test is suitable for film thicknesses up to 250 μm. The X-cut test is not limited by thickness.
For hard coatings, it might not be possible to use the cross-cut test, in which case the X-cut test should be
used.
For coatings containing pigments that have a flake format, the assessment of either the cross-cut or the X-cutmight be misleading. The coating manufacturer should be consulted for recommendations.

作者: hepe32    时间: 2012-9-12 16:37
防腐配套产品通常都是用拉拔测试附着的
作者: zerozsh    时间: 2012-9-15 09:21
一般不建议这么做的,这种涂料一般做pull off好一点
作者: shashou    时间: 2012-9-28 08:49
本帖最后由 shashou 于 2012-9-28 08:50 编辑

都可以划格,在多厚的情况下,就是看几级,富锌容易厚涂,所以富着总感觉不好,一般使用拉开法
作者: 牛振军    时间: 2012-11-6 15:21
环氧富锌一定能通过,无机富锌要选择好的粘合剂才可以
作者: FCAB    时间: 2012-11-21 18:12
本帖最后由 FCAB 于 2012-11-21 18:15 编辑

在环境温度为5-10度的条件下,用划格法检测附着力,划格区域用胶带纸粘成片脱落,但再在其它地方将漆膜随意划破一道(划透到底材),然后用手使劲抠漆膜都不掉,有人知道是什么原因吗?
作者: 武汉昱奥    时间: 2012-11-21 21:54
shigang2006 发表于 2011-11-25 13:38
为什么我做的醇溶性无机富锌底漆表面很粗糙呢 且附着力不好

主要是颜料浆组份的配方的问题,说白了是树脂和颜料配比的问题。还有你是用的什么填料,哪里的树脂等?这都有关系的。你可以跟我联系一下,我是专业做这的!
作者: 武汉昱奥    时间: 2012-11-21 21:57
无机富锌应该用拔开法
作者: 牛振军    时间: 2012-11-24 16:09
都可以做,问题是无机富锌树脂选择不当就难通过
作者: lqyzq123    时间: 2012-11-24 16:59
可以画格。。。我做过,监理要求的,不够厚度要小于80,不然容易脱落,再就是喷的时候要一边搅一边用无气喷涂喷。。效果不错。。0级。
作者: 武汉昱奥    时间: 2012-11-25 20:35
肯定是用拉开法,国家已有无机富锌漆附着力的检测标准了-------拉开法。
作者: greatlghqm    时间: 2016-5-31 10:33
众说纷纭,但是主要还是要看客户的技术要求吧。
作者: mengjie1019    时间: 2016-6-13 09:25
shigang2006 发表于 2011-11-25 13:38
为什么我做的醇溶性无机富锌底漆表面很粗糙呢 且附着力不好

调整你的溶剂组成,应该是溶剂挥发过快造成的
作者: chenzeyang1988    时间: 2016-6-22 11:29
12楼正解,好像都是拉开法比较多吧,国标也有明确规定